ELECTROMAGNETIC CONDUCTIVE COATING APPLICATION continued
(9) Brush application: Brush the surface with conductive coating material. Overlap edge of damaged area
approximately 0.75 INCH where possible (first pass should completely wet the surface). Allow 2 to 10
MINUTES before re-painting to complete the first coat. Dry for 30 MINUTES to 2 HOURS before applying
a second coat. Use brush (item 36, App F) and corrosion resistant coating (item 65, App F).
(10) Apply a second coat of conductive coating. Use corrosion resistant coating (item 65, App F). Proceed to
step (12).
NOTE
Paint shall be applied with a pressure of 10 to 20 PSI. It is important to agitate paint mixture every 2 to
3 minutes to keep the conductive fillers suspended in the paint solution.
(11) Spray application: Apply a uniform coat of the conductive coating by spraying four to five even passes over
component surface from a distance of 6 to 10 INCHES. Use corrosion resistant coating (item 65, App F).
(12) Apply curing criteria in paragraph 2.34.4.e.
d. Inspect (QA).
END OF TASK